A carton of eye patch sachets that leaks at the corner after a month at sea is one of the more expensive complaints a factory handles, because the whole pallet is suspect. In most cases the film is fine and the seal is marginal: strong enough to pass a visual check, too weak to survive handling.

1. What Fails First

Seals fail before films do. A seal is a weld across a contaminated or under-heated interface, and a channel a fraction of a millimetre wide is enough. Water then travels by capillary action along the channel, which is why a leaker often shows a damp patch several centimetres from the visible defect.

2. The Number to Ask For

Peel strength is reported in newtons per 15 mm of seal width. Laminates with an aluminium layer typically sit between 1.5 and 3.0 N/15 mm; below about 1.2 N the seal opens under handling, and above 3.5 N the film can tear or delaminate when the consumer opens it. Ask for the mean and the lowest single value from ten specimens.

3. Three Variables, One Window

Sealing temperature, dwell time and jaw pressure interact. A typical laminate window is 140-160 C, 0.3-0.5 seconds and 0.3-0.5 MPa, but the window belongs to the film structure, not to a general rule. Move temperature up and dwell can come down; move pressure up without temperature and the seal looks tight and peels weakly.

4. Contamination in the Seal Zone

A film of serum 0.05 mm thick across the seal area halves peel strength. Fill volume that reaches the seal, splashing on a fast line, and powder from a scrub are the usual sources. A 3-5 mm clear margin between product and seal, with a nitrogen or air puff to clear the zone, fixes most of it.

5. Peel Test or Burst Test

The two answer different questions. Peel measures the weld; burst measures the whole pack and is closer to what happens in a carton. Run both: burst at 0.6-1.0 bar above ambient for a small sachet, and peel on a tensile frame at 300 mm per minute. A pack that bursts well but peels weakly has a seal that will creep under load.

6. Why Eye Patches Are Harder

A hydrogel patch is thick, wet and curved, and it presses against the seal from inside. Fill weights of 4-8 g in a small pouch leave little headspace, so any product in the seal zone is under pressure from the moment the pouch is closed. Curved patches also demand a wider seal than a flat sheet mask of the same area.

7. Ageing the Seal

Seal strength is not constant. Three months at 40 C and 75% relative humidity, or six weeks at 50 C, will often drop peel strength 15-30% as plasticiser migrates and the weld relaxes. A seal that reads 2.0 N on the fill day and 1.4 N after ageing is the classic transport failure. Test aged, not fresh.

8. Line Audits

Pull three sachets every 30 minutes from each lane and record burst pressure plus a visual check of the seal band. Measure jaw temperature with a contact probe, not an infrared gun, because the emissivity of a coated jaw reads low. Log the values in the batch record; a drift of 5 C across a shift is common and invisible.

9. Fixing a Marginal Seal

In order of cost: raise dwell slightly, clean the jaw with a brass brush each shift, increase the clear margin, switch to a film with a wider seal window. A change of jaw coating or a duplex structure is the expensive route and rarely needed. Whatever is done, re-run the peel test aged, not on the day of the change.

10. Where it fits

Seal integrity ties the film, the fill and the machine together. Review pouch formats in products, read related quality notes in news, and check the material background in the encyclopedia. For patch formats such as eye patches, specify peel strength after ageing.

Keep reading

More from the plant floor

All news

Start a project

Ready to put your name on a formula?

Send a brief and our formulation team will come back with a costed proposal, sample plan and timeline — typically within two working days.